Dyeing and Colour Guides for Polyester Knits
The colour of a polyester knit is settled in three steps. Disperse dye is diffused at high temperature into a fibre whose glass transition has been passed. Reductive clearing then removes unfixed surface dye and secures fastness. Finally, colour is approved against a spectrophotometric ΔE value under defined lighting. These four guides explain each step and how to specify it.
This category brings together the chain that runs from dyeing a polyester knit to approving its colour. Polyester is a hydrophobic, chemically inert fibre, so it is dyed only with disperse dyes and never with reactive or direct dyes. Buyers and product developers make several decisions along this chain. The dyeing route is chosen by fibre blend and equipment, and the dye energy class by the highest thermal process the product will face. Fastness targets are written with the ISO 105 test methods. The colour tolerance enters the contract together with its formula, illuminant and limit.
The four guides follow the order of work in the dyehouse. Start with why polyester is dyed with disperse dyes at high temperature, then read how the HT/HP, carrier and thermosol routes work. The third guide covers reductive clearing, the white specks caused by oligomer and how fastness is proven with ISO 105 tests. The last guide explains how colour difference is measured as ΔE and under which conditions a lab-dip approval is written.
Decisions made in this category
| Decision | What to check |
|---|---|
| Which dyeing route suits the fabric? | HT/HP exhaust at ~130 °C in a pressurised vessel, carrier dyeing at ~95–100 °C for heat-sensitive blends such as elastane, thermosol for continuous high-volume work The Disperse Dyeing Process: HT/HP, Thermosol and Carrier |
| Which disperse dye energy class is chosen? | The highest thermal process the product will face (heat-setting, pleating, transfer printing) rather than the shade, and the balance between diffusion rate and sublimation fastness across the E, SE and S classes How Polyester Is Dyed: Disperse Dyes and HT |
| How is a level dyeing secured? | A heating ramp slowed through the ~100–120 °C critical zone (typically 1–1.5 °C/min), the hold time at 130 °C and a bath pH of 4.5–5.5 set with an acetic acid/acetate buffer The Disperse Dyeing Process: HT/HP, Thermosol and Carrier |
| Is reductive clearing needed after dyeing? | Depth of shade and the wet-rub and wash grades, together with the classic alkaline recipe of sodium dithionite and caustic soda, typically 70–80 °C for 10–20 minutes Reductive Clearing, Oligomers and Wash Fastness |
| Which fastness tests go into the specification? | ISO 105-C06 washing, ISO 105-E04 perspiration and ISO 105-X12 dry and wet rubbing assessed on the 1–5 grey scales, and ISO 105-B02 light fastness on the blue wool 1–8 scale Reductive Clearing, Oligomers and Wash Fastness |
| How is colour tolerance written into the contract? | The formula and ratio (CMC 2:1 or CIEDE2000), the D65/10° reference and a component tolerance for ΔL*, ΔC* and ΔH* instead of a single number Color Management and Delta E in Polyester Knits |
| Why does colour look different under store lighting? | Metamerism, assessed under several illuminants such as D65, TL84 and A, and the CIE metamerism index (MI > 1.0 points to a different dye combination) Color Management and Delta E in Polyester Knits |
Key facts
- PET’s glass-transition temperature is ~80 °C dry and around ~65 °C in water. HT/HP exhaust dyeing runs at ~130 °C under pressure, while carrier dyeing does the same work at ~95–100 °C. How Polyester Is Dyed: Disperse Dyes and HT
- The highest thermal process the product will face dictates the energy class, not the shade. High-energy (S) dyes are chosen for products requiring thermosol and 180–200 °C heat-setting. How Polyester Is Dyed: Disperse Dyes and HT
- In HT/HP exhaust the bath is taken to ~130 °C in a closed system. The saturated steam pressure at that temperature is on the order of 2–3 bar, and the hold commonly lasts ~30–60 min. The Disperse Dyeing Process: HT/HP, Thermosol and Carrier
- The bath pH is set to 4.5–5.5 with an acetic acid/acetate buffer. Low pH is critical both for dispersant stability and to prevent hydrolytic breakdown of the azo chromophores. The Disperse Dyeing Process: HT/HP, Thermosol and Carrier
- Classic reductive clearing uses sodium dithionite and caustic soda in an alkaline bath, typically at 70–80 °C for 10–20 minutes. The effect matters most on deep shades, because the amount of surface-held dye grows with depth of shade. Reductive Clearing, Oligomers and Wash Fastness
- PET fibre carries roughly 1–3% low-molecular-weight oligomer, dominated by the cyclic trimer. Draining the bath after the HT step above the re-crystallisation threshold (typically ≥70–80 °C) reduces surface deposition. Reductive Clearing, Oligomers and Wash Fastness
- A well-cleared deep shade is expected to land at 4–4/5 in wash and dry rub and at 3/4–4 in wet rub. Wet rub usually sits half to one grade below dry. Reductive Clearing, Oligomers and Wash Fastness
- A common textile practice holds the total difference between lab-dip and bulk at roughly ΔE ≤ 1.0, up to 1.5 for some end uses. This is a limit the brand sets, not a universal rule. Color Management and Delta E in Polyester Knits
Reading order
- How Polyester Is Dyed: Disperse Dyes and HT — Polyester cannot be dyed with reactive dyes because PET is hydrophobic and chemically inert; the only route is diffusing water-insoluble disperse dye into the fibre’s amorphous regions. That requires passing the glass transition (~80 °C dry, ~65 °C in water): HT/HP exhaust dyeing runs at ~130 °C under pressure, while carrier dyeing does the same work at ~95–100 °C.
- The Disperse Dyeing Process: HT/HP, Thermosol and Carrier — Dyeing polyester is the engineering of placing a near-water-insoluble disperse dye into the amorphous regions of a fibre whose glass-transition temperature has been exceeded, by solid-state diffusion. Chemical compliance is governed by ZDHC and OEKO-TEX, and fastness by the ISO 105 series.
- Reductive Clearing, Oligomers and Wash Fastness — After disperse dyeing, unfixed surface dye and migrating cyclic oligomer wreck fastness and appearance unless reductive clearing removes them. The result shows directly in ISO 105 wash and rub fastness grades.
- Color Management and Delta E in Polyester Knits — Colour consistency is not an eyeball call but a measured number: the difference between two colours is expressed as ΔE, and today’s standard is CIEDE2000 (CIE 142-2001 · ISO/CIE 11664-6). Lab-dip approval sets the threshold for that metric; metamerism — two colours matching under one illuminant and diverging under another — is why approval always happens under a defined light source.
Frequently asked questions
Can I buy undyed (ecru) fabric for printing?
Yes. We sell undyed (ecru) fabric for printing. State the fabric type, weight and width in your request.